Product name:KN-816C3
 
Classification:A5.5 / E8016-C3
 
 

  1. It is suitable for welding 540N/mm2 grade steel for low temperature resistance.
  2. It provides superior weldability and X-ray quality welds.
  3. Weld metal contains 1.1%Ni-0.25%Mo and good impact properties at -40°C.
  4. It is ideal for welding in LNG storage tanks or 1%Ni steel for low temperature resistance.

 

Welding Position

All Positions

Welding Instruction

(1) Clean up the contaminations on the steel.

(2) Dry the electrodes at 350~400°C for 60 minutes before welding.

(3) Keep arc as short as possible. Take the back step method to prevent porosity at arc start and re-start. (Please refer to Appendix A)

(4) High heat input will lower the impact value. Please carefully select the welding current.

(5) The preheat temperature for thick plate is 50~100°C.

Typical Chemical Composition of Weld Metal (wt %)

C

Si

Mn

P

S

Ni

 

0.060

0.52

0.88

0.010

0.008

0.93

 

Typical Mechanical Properties of Weld Metal (As welded)

Tensile Strength

N/mm2(kgf/mm2)

Yield Strength

N/mm2(kgf/mm2)

Elongation

%

Charpy V-Notch

°C

J (kgf -m)

560(57.1)

490(50.0)

32

0

-40

118(12.0)

Size and Suggested Operating Range (AC or DC+)

Diameter (mm) x Length(mm)

2.6x300

3.2x350

4.0x400

5.0x400

 

Amp

H

70~100

100~140

140~180

180~230

 

V-up/OH

60~90

90~130

120~160

 


No.8, Luke 3rd Rd., Luzhu Dist., Kaohsiung City 821, Taiwan (R.O.C.)      TEL:886-7-6955155      FAX:886-7-6955166

Copyright (C) Kuang Tai Metal Industrial Co., Ltd. All Rights Reserved.   Designed by GRNET