KF-300S/KW-316L
Basicity: 2.5
The weld metal has a low-carbon austenitic structure containing 18.5% Cr, 12.5% Ni, and 2.5% Mo.
Basicity: 2.5
The weld metal has a low-carbon austenitic structure containing 18.5% Cr, 12.5% Ni, and 2.5% Mo.
| AWS A5.9/A5.9M | ER316L |
| JIS Z3323 | YS316L |
| EN ISO 14343-A | S 19 12 3 L |
| YB T5092 | H022Cr19Ni12Mo2 |
Please refer to the precautions for submerged arc welding (SAW).
It is suitable for welding critical chemical containers, and is particularly effective for LNG vessels where low-temperature impact toughness is required.
| C | Si | Mn | P | S | Cr | Ni | Mo |
| 0.02 | 0.42 | 1.91 | 0.012 | 0.009 | 19.14 | 12.63 | 2.53 |
| Tensile Strength N/mm² | Yield Strength N/mm² | Elongation % |
| 546 | 377 | 39 |
| Diameter(mm) | 2.0 | 2.4 | 3.2 |
| Current(A) | 190~300 | 275~350 | 350~450 |